ELECTRONIC SPACE PRODUCTS INTERNATIONAL


1050 Benson Way, Ashland, OR 97520

Toll Free (800) 638-2581 * Fax (541) 488-8313

E-Mail: sales@espimetals.com

 

 

Inconel 600

 

 

 

              Inconel 600 is a nickel-chromium alloy with good oxidation resistance at high temperatures and resistance to chloride ion stress-corrosion cracking, corrosion by high-purity water, and caustic corrosion. Used for furnace components, in chemical and food process-ing, in nuclear engineering, and for sparking electrodes.

 

 

Typical Analysis in Percent:

 

              Ni (+Co):             72                        Cr:                       14 - 17

              Fe:                       6 - 10                   C:                         .15

              Mn:                      1                          Si:                        .5

              Cu:                       .5

 

 

Physical Properties:

 

Density: 8.47 g/cm3

 

Melting Point/Range: 1355 - 1413 oC (2470 - 2575 oF)

 

                                                                                      J/kg ⋅ K                             Btu/lb ⋅ oF

Specific Heat:                                                              444                                     0.106

 

                                                                                      µm/m ⋅ K                           µin/in ⋅ K

Average Coefficient of Thermal Expansion:            13.3                                    7.4

 

                                                                                      W/m ⋅ K                            Btu ⋅ in./ft2 ⋅ h ⋅ oF

Thermal Conductivity:                                               14.9                                    103

 

                                                                                      % IACS                            nΩ ⋅ m

Electrical Resistivity:                                                  1.7                                      1030

 

Magnetic Permeability: 1.010

 

Curie Temperature: -124 oC (-192 oF)

 

 

Typical Mechanical Properties:

 

At Room Temperature:

 

                            Ultimate Tensile                 Yield Strength                Elongation in                  Elastic Modulus

                                Strength                            (0.2 % offset)                  50 mm (2")                     (Tension)

                            MPa             ksi                  MPa        ksi                             %                            GPa        106 psi

                            655               95                   310          45                              40                            207           30

 

Hardness: 75 HRB